QT400-18 Ductile Cast Iron Casting Material

Ductile Cast Iron

Download MDS PDF · Request a Quote

Introduction

GB/T 1348 Grade QT400-18 is a spheroidal graphite iron casting grade. Process options include sand casting, shell molding and lost-foam casting. Typical uses include pump housings, valve bodies, bearing supports and equipment brackets.

FieldValue
DesignationQT400-18
Material TypeCast Iron
Sub TypeDuctile Cast Iron
Product Formcasting

Manufacturing Process

Sand Casting
Shell Molding Casting
Lost Foam Casting

Equivalent Materials

StandardMaterial Grade
SAE J434D400
EN 1563EN-GJS-400-18
ASTM A53660-40-18
ISO 1083ISO1083/JS/400-18

Approximate materials; not guaranteed interchangeable.

Similar Materials

Not Available

Reference Standards

StandardStandard TitleEditionSpecification
GB/T 1348Spheroidal graphite iron castings2019QT400-18

Physical Properties

PropertyValueApplicable Conditions
Density7.1 kg/dm³[1]Room temperature unless otherwise stated
Elastic Modulus169 GPa[1]Room temperature unless otherwise stated
Poisson Ratio0.275[1]Room temperature unless otherwise stated
Thermal Conductivity36.2 W/(m·K)[1]Test temperature: 300 °C
Specific Heat515 J/(kg·K)[1]Temperature range: 20–500 °C
Thermal Expansion12.5 ×10⁻⁶/K[1]Temperature range: 20–400 °C
Electrical Resistivity0.5 µΩ·m[1]Room temperature unless otherwise stated
Hysteresis Loss600 J/m³[1]Room temperature unless otherwise stated; B = 1 T
Matrix StructureFerritic; informative Table G.1 matrix description, not a prescribed heat-treatment schedule.[1]
Maximum Magnetic Permeability2136 µH/m[1]Room temperature unless otherwise stated

Notes

  • [1] Informative values; not mandatory acceptance limits.

Chemical Composition

No specified chemical composition limits in GB/T 1348

Heat Treatment

General casting and chemical requirements — No grade-specific heat-treatment temperature or holding schedule is prescribed. Alloy adjustment or heat treatment may control the ferrite/pearlite ratio (6.2). When heat treatment is required, test blocks receive the same treatment as the represented castings; cast-on blocks remain attached until after heat treatment unless agreed otherwise (8.1.6; 8.2.3.5; 8.2.5.5). Repeated heat treatments for retesting shall not exceed two (10.5.3).

Mechanical Properties

Primary Mechanical Properties

GB/T 1348 — 2019

Condition: Table 1; Separately cast, cast-on or side-by-side cast sample; 30 < t ≤ 60 mm; normative; 30 < t ≤ 60 mm

PropertyRequirement
Yield Strength (Rp0.2)≥ 250 MPa[1][2][3][4]
Tensile Strength≥ 390 MPa[1][2][3][4]
Elongation≥ 15 %[1][2][3][4]

Notes

  • [1] Table 1: results from cast samples do not directly represent casting-body properties. Separately cast, cast-on and side-by-side cast samples are covered. L denotes low temperature and R room temperature. Elongation is measured at original gauge length L0=5d; alternate gauge lengths require the provisions of 9.1 and normative Annex D.
  • [2] Gauge Length: L0 = 5d
  • [3] GB/T 228.1
  • [4] Minimum prescribed value

GB/T 1348 — 2019

Condition: Table 1; Separately cast, cast-on or side-by-side cast sample; 60 < t ≤ 200 mm; normative; 60 < t ≤ 200 mm

PropertyRequirement
Yield Strength (Rp0.2)≥ 240 MPa[1][2][3][4]
Tensile Strength≥ 370 MPa[1][2][3][4]
Elongation≥ 12 %[1][2][3][4]

Notes

  • [1] Table 1: results from cast samples do not directly represent casting-body properties. Separately cast, cast-on and side-by-side cast samples are covered. L denotes low temperature and R room temperature. Elongation is measured at original gauge length L0=5d; alternate gauge lengths require the provisions of 9.1 and normative Annex D.
  • [2] Gauge Length: L0 = 5d
  • [3] GB/T 228.1
  • [4] Minimum prescribed value

GB/T 1348 — 2019

Condition: Table 1; Separately cast, cast-on or side-by-side cast sample; t ≤ 30 mm; normative; t ≤ 30 mm

PropertyRequirement
Yield Strength (Rp0.2)≥ 250 MPa[1][2][3][4]
Tensile Strength≥ 400 MPa[1][2][3][4]
Elongation≥ 18 %[1][2][3][4]

Notes

  • [1] Table 1: results from cast samples do not directly represent casting-body properties. Separately cast, cast-on and side-by-side cast samples are covered. L denotes low temperature and R room temperature. Elongation is measured at original gauge length L0=5d; alternate gauge lengths require the provisions of 9.1 and normative Annex D.
  • [2] Gauge Length: L0 = 5d
  • [3] GB/T 228.1
  • [4] Minimum prescribed value

GB/T 1348 — 2019

Condition: Table C.1; Specimen cut from the casting; source designation QT400-18/C; sampling position and acceptance properties subject to agreement; 30 < t ≤ 60 mm; informative; 30 < t ≤ 60 mm

Informative

PropertyValue
Yield Strength (Rp0.2)≥ 240 MPa[1][2][3][4][5][6]
Tensile Strength≥ 370 MPa[1][2][3][4][5][6]
Elongation≥ 12 %[1][2][3][4][5][6]

Notes

  • [1] informative 30 < wall thickness ≤ 60 mm
  • [2] Gauge Length: L0 = 5d
  • [3] GB/T 228.1
  • [4] Informative minimum guideline, not an unconditional acceptance requirement
  • [5] Informative reference value
  • [6] not an acceptance requirement

GB/T 1348 — 2019

Condition: Table C.1; Specimen cut from the casting; source designation QT400-18/C; sampling position and acceptance properties subject to agreement; 60 < t ≤ 200 mm; informative; 60 < t ≤ 200 mm

Informative

PropertyValue
Yield Strength (Rp0.2)≥ 230 MPa[1][2][3][4][5][6]
Tensile Strength≥ 350 MPa[1][2][3][4][5][6]
Elongation≥ 10 %[1][2][3][4][5][6]

Notes

  • [1] informative 60 < wall thickness ≤ 200 mm
  • [2] Gauge Length: L0 = 5d
  • [3] GB/T 228.1
  • [4] Informative minimum guideline, not an unconditional acceptance requirement
  • [5] Informative reference value
  • [6] not an acceptance requirement

GB/T 1348 — 2019

Condition: Table C.1; Specimen cut from the casting; source designation QT400-18/C; sampling position and acceptance properties subject to agreement; t ≤ 30 mm; informative; t ≤ 30 mm

Informative

PropertyValue
Yield Strength (Rp0.2)≥ 250 MPa[1][2][3][4][5][6]
Tensile Strength≥ 390 MPa[1][2][3][4][5][6]
Elongation≥ 15 %[1][2][3][4][5][6]

Notes

  • [1] informative wall thickness ≤ 30 mm
  • [2] Gauge Length: L0 = 5d
  • [3] GB/T 228.1
  • [4] Informative minimum guideline, not an unconditional acceptance requirement
  • [5] Informative reference value
  • [6] not an acceptance requirement

GB/T 1348 — 2019

Condition: Table G.1; informative

Informative

PropertyValue
Shear Strength360 MPa[1][2][3][4]
Compressive Strength700 MPa[1][2][3][4]

Notes

  • [1] Annex G informative reference data
  • [2] measured at room temperature unless otherwise stated, not an acceptance limit
  • [3] Informative reference value
  • [4] not an acceptance requirement

GB/T 1348 — 2019

Condition: t ≤ 30 mm; Table G.2; Specimen cut from casting; diameter ≤25 mm; t ≤ 30 mm; informative

Informative

PropertyValue
Tensile Strength400 MPa[1][2][3][4][5]

Notes

  • [1] Informative guideline
  • [2] stress-controlled fatigue
  • [3] N = 10^7 cycles, failure probability P = 50% for fatigue data
  • [4] not an acceptance requirement
  • [5] Informative reference value

Additional Mechanical Properties

GB/T 1348 — 2019

Other Mechanical Properties

Condition: Table G.1; informative

Informative

PropertyValue
Torsional Strength360 MPa[1][2][3][4]

Notes

  • [1] Annex G informative reference data
  • [2] measured at room temperature unless otherwise stated, not an acceptance limit
  • [3] Informative reference value
  • [4] not an acceptance requirement

GB/T 1348 — 2019

Fracture Toughness

Condition: Table G.1; informative

Informative

PropertyValue
Fracture Toughness (KIC)30 MPa√m[1][2][3][4]

Notes

  • [1] Annex G informative reference data
  • [2] measured at room temperature unless otherwise stated, not an acceptance limit
  • [3] Informative reference value
  • [4] not an acceptance requirement

GB/T 1348 — 2019

Fatigue Properties

Condition: t ≤ 30 mm

Informative

PropertyValue
Notched Rotating Bending Fatigue Strength128 MPa[1][2][3][4][5][6][7][8][9][10][11][12][13][14][15][16]
Notched Rotating Bending Fatigue Ratio0.32[1][2][3][4][5][6][7][8][9][10][11][17]
Reversed Tension Compression Fatigue Strength168 MPa[1][3][4][5][6][7][8][9][10][11][12][16][18][19][20]
Reversed Tension Compression Fatigue Ratio0.42[1][3][4][5][6][7][8][9][10][11][17][18]
Pulsating Tension Fatigue Strength235 MPa[1][3][4][5][6][7][8][9][10][11][16][18][21][22][23][24]
Reversed Torsional Fatigue Strength152 MPa[1][3][4][5][6][7][8][9][10][11][12][16][18][25][26]
Reversed Torsional Fatigue Ratio0.38[1][3][4][5][6][7][8][9][10][11][17][18]
Rotating Bending Fatigue Strength188 MPa[1][3][4][5][6][7][8][9][10][11][12][16][18][27][28]
Rotating Bending Fatigue Ratio0.47[1][3][4][5][6][7][8][9][10][11][17][18]

Notes

  • [1] GB/T 1348:2019 G.2 prints contradictory cycle wording. With owner authorization, adopt 10 million cycles (N=10^7), P=50% from verified ISO 1083:2018 G.2 footnotes b/c. This is separately sourced supporting clarification, not an official amendment or mandatory acceptance value.
  • [2] Notched Rotating Bending Fatigue Strength; Notched Rotating Bending Fatigue Ratio: Notched specimen, Kt ≤3 machined from a sample cut from casting
  • [3] diameter ≤25 mm
  • [4] relevant wall thickness t ≤30 mm
  • [5] informative wall thickness ≤ 30 mm
  • [6] Informative guidance, not an acceptance requirement
  • [7] GB cycle wording retained as inconsistent
  • [8] N = 10^7 cycles (10 million), P = 50% adopted from ISO 1083:2018 G.2 footnotes b/c under owner authorization
  • [9] Stress-controlled fatigue according to Wöhler
  • [10] Informative reference value
  • [11] not an acceptance requirement
  • [12] Notched Rotating Bending Fatigue Strength; Reversed Tension Compression Fatigue Strength; Reversed Torsional Fatigue Strength; Rotating Bending Fatigue Strength: R = -1
  • [13] Notched Rotating Bending Fatigue Strength: approximately 21.8%
  • [14] Notched Rotating Bending Fatigue Strength: Kt ≤ 3
  • [15] Notched Rotating Bending Fatigue Strength: σbwk(R=-1)/Rm ≈ 0.40 - 0.0002 × Rm
  • [16] Notched Rotating Bending Fatigue Strength; Reversed Tension Compression Fatigue Strength; Pulsating Tension Fatigue Strength; Reversed Torsional Fatigue Strength; Rotating Bending Fatigue Strength: Mean source-table reference strength, not a guaranteed limit
  • [17] Notched Rotating Bending Fatigue Ratio; Reversed Tension Compression Fatigue Ratio; Reversed Torsional Fatigue Ratio; Rotating Bending Fatigue Ratio: Source-table ratio, not a calculated value
  • [18] Reversed Tension Compression Fatigue Strength; Reversed Tension Compression Fatigue Ratio; Pulsating Tension Fatigue Strength; Reversed Torsional Fatigue Strength; Reversed Torsional Fatigue Ratio; Rotating Bending Fatigue Strength; Rotating Bending Fatigue Ratio: Unnotched specimen machined from a sample cut from casting
  • [19] Reversed Tension Compression Fatigue Strength: approximately 22.3%
  • [20] Reversed Tension Compression Fatigue Strength: σw/Rm ≈ 0.50 - 0.0002 × Rm
  • [21] Pulsating Tension Fatigue Strength: R = 0
  • [22] Pulsating Tension Fatigue Strength: σmax = 2σ
  • [23] Pulsating Tension Fatigue Strength: approximately 9%
  • [24] Pulsating Tension Fatigue Strength: σ(R=0)/σ(R=-1) ≈ 0.7
  • [25] Reversed Torsional Fatigue Strength: approximately 14%
  • [26] Reversed Torsional Fatigue Strength: τw/Rm ≈ 0.46 - 0.0002 × Rm
  • [27] Rotating Bending Fatigue Strength: approximately 14.2%
  • [28] Rotating Bending Fatigue Strength: σw/Rm ≈ 0.55 - 0.0002 × Rm

Welding Conditions

Not Available

Applications

Ductile iron GB/T 1348 Grade QT400-18 is used for pump housings, valve bodies, bearing supports and equipment brackets. These castings are found in fluid-handling equipment, agricultural machinery and general mechanical assemblies. Selection within this family depends on the actual component geometry and loading. Pipes, pipe fittings and associated joints are outside this standard; pressure-retaining machinery parts require the applicable component specification and inspection requirements.

Need QT400-18 Castings?

Contact us for casting and machining inquiries.

Last Updated: November 25, 2026

error: Alert: Thanks for your interesting, but Article is protected ! You can click the Top Right email!