ISO1083/JS/800-2 Ductile Cast Iron Casting Material

Ductile Cast Iron

Download MDS PDF · Request a Quote

Introduction

ISO1083/JS/800-2 is a ductile cast iron designated under ISO 1083. The standard reports pearlite or tempered martensite as a typical matrix. Typical family castings include bearing housings and pump components.

FieldValue
DesignationISO1083/JS/800-2
Material TypeCast Iron
Sub TypeDuctile Cast Iron
Product Formcasting

Manufacturing Process

Sand Casting
Shell Molding Casting
Lost Foam Casting

Equivalent Materials

StandardMaterial Grade
NBN 830-02FNG80-2
IS 1865SG800/2
SAE J434D800
EN 1563EN-GJS-800-2
AS 1831800-2
NF A32-201FGS800-2
UNE 36-118FGE80-2
BS 2789800/2
NS11 301SJK-800
UNI 4544GS800-2
JIS G5502FCD800
SS 14 070864-03
ASTM A536120-90-02
DIN 1693-1GGG-80
GB/T 1348QT800-2

Approximate materials; not guaranteed interchangeable.

Similar Materials

Not Available

Reference Standards

StandardStandard TitleEditionSpecification
ISO 1083Spheroidal graphite cast irons — Classification2018ISO1083/JS/800-2

Physical Properties

PropertyValueApplicable Conditions
Density7.2 kg/dm³[2]Room temperature unless otherwise specified
Elastic Modulus176 GN/m²[2]Room temperature unless otherwise specified
Poisson Ratio0.275[2]Room temperature unless otherwise specified
Thermal Conductivity31.1 W/(m·K)[2]Test temperature: 300 °C
Specific Heat515 J/(kg·K)[2]Temperature range: 20–500 °C
Thermal Expansion12.5 µm/(m·K)[2]Temperature range: 20–400 °C
Electrical Resistivity0.54 µΩ·m[2]Room temperature unless otherwise specified
Hysteresis Loss2700 J/m³[2]Hysteresis loss at B = 1 T; Room temperature unless otherwise specified
Matrix Structurepearlite or tempered martensite[1][2]
Maximum Magnetic Permeability501 µH/m[2]Room temperature unless otherwise specified

Notes

  • [1] Matrix Structure: Typical structure
  • [2] Informative values; not mandatory acceptance limits.

Chemical Composition

Not Available

Heat Treatment

ISO 1083–2018

Not Available

Mechanical Properties

Primary Mechanical Properties

ISO 1083 — 2018

Condition: t ≤ 30 mm

PropertyRequirement
Yield Strength (Rp0.2)≥ 480 MPa[1][2][3]
Tensile Strength≥ 800 MPa[1][2][3]
Elongation≥ 2 %[1][2][3][4][5]

Notes

  • [1] Separately cast, cast-on or side-by-side cast samples
  • [2] Values apply to sand moulds or moulds of comparable thermal behaviour
  • [3] alternative processes are subject to amendments agreed in the order.
  • [4] Elongation: Elongation values determined from L0 = 5 d
  • [5] Elongation: other gauge lengths see 9.1 and Annex B.

ISO 1083 — 2018

Condition: t ≤ 30 mm

Informative

PropertyValue
Yield Strength (Rp0.2)≥ 460 MPa[1][2][3]
Tensile Strength≥ 780 MPa[1][2][3]
Elongation≥ 2 %[1][2][3][4]

Notes

  • [1] test pieces machined from samples cut from castings
  • [2] Informative reference value
  • [3] not an acceptance requirement
  • [4] Elongation: For elongation results, the reference gauge length is L0 = 5 d.

ISO 1083 — 2018

Informative

PropertyValue
Shear Strength720 MPa[1][2][3]
Compressive Strength1150 MPa[1][2][3]

Notes

  • [1] Room temperature unless otherwise specified.
  • [2] Informative reference value
  • [3] not an acceptance requirement

ISO 1083 — 2018

Informative

PropertyValue
Tensile Strength800 MPa[1][2][3][4]

Notes

  • [1] specimens diameter <=25 mm from casting
  • [2] relevant wall thickness <=30 mm
  • [3] Informative reference value
  • [4] not an acceptance requirement

Additional Mechanical Properties

ISO 1083 — 2018

Other Mechanical Properties

Informative

PropertyValue
Torsional Strength720 MPa[1][2][3]

Notes

  • [1] Room temperature unless otherwise specified.
  • [2] Informative reference value
  • [3] not an acceptance requirement

ISO 1083 — 2018

Fatigue Properties

Informative

PropertyValue
Reversed Tension Compression Fatigue Strength272 MPa[1][2][3][4][5][6]
Reversed Tension Compression Fatigue Ratio0.34[1][2][3][4][5][6]
Pulsating Tension Fatigue Strength381 MPa[1][2][3][4][5][6]
Reversed Torsional Fatigue Strength240 MPa[1][2][3][4][5][6]
Reversed Torsional Fatigue Ratio0.30[1][2][3][4][5][6]
Rotating Bending Fatigue Strength312 MPa[1][2][3][4][5][6]
Rotating Bending Fatigue Ratio0.39[1][2][3][4][5][6]
Notched Rotating Bending Fatigue Strength192 MPa[1][2][4][5][6][7]
Notched Rotating Bending Fatigue Ratio0.24[1][2][4][5][6][7]

Notes

  • [1] specimens diameter <=25 mm from casting
  • [2] relevant wall thickness <=30 mm
  • [3] Reversed Tension Compression Fatigue Strength; Reversed Tension Compression Fatigue Ratio; Pulsating Tension Fatigue Strength; Reversed Torsional Fatigue Strength; Reversed Torsional Fatigue Ratio; Rotating Bending Fatigue Strength; Rotating Bending Fatigue Ratio: Unnotched specimen
  • [4] 10 million cycles and 50% failure probability.
  • [5] Informative reference value
  • [6] not an acceptance requirement
  • [7] Notched Rotating Bending Fatigue Strength; Notched Rotating Bending Fatigue Ratio: Notched specimen with stress concentration factor Kt ≤ 3

Welding Conditions

Not Available

Applications

Ductile iron ISO1083/JS/800-2 belongs to the spheroidal graphite iron casting family. Typical products of the wider ductile-iron family include transmission components, hubs, brackets and housings for pumps and bearings. Examples of end-use sectors include general industrial machinery, agriculture, construction and pump equipment.

Need ISO1083/JS/800-2 Castings?

Contact us for casting and machining inquiries.

Last Updated: November 16, 2026

error: Alert: Thanks for your interesting, but Article is protected ! You can click the Top Right email!