ISO1083/JS/500-7 Ductile Cast Iron Casting Material
Ductile Cast Iron
Introduction
ISO1083/JS/500-7 is a spheroidal graphite iron casting material in ISO 1083. The standard reports ferrite-pearlite as a typical matrix. Family applications include hubs and gears in agricultural and industrial machinery.
| Field | Value |
|---|---|
| Designation | ISO1083/JS/500-7 |
| Material Type | Cast Iron |
| Sub Type | Ductile Cast Iron |
| Product Form | casting |
Manufacturing Process
Sand Casting
Shell Molding Casting
Lost Foam Casting
Equivalent Materials
| Standard | Material Grade |
|---|---|
| NBN 830-02 | FNG50-7 |
| NS11 301 | SJK-500 |
| NF A32-201 | FGS500-7 |
| EN 1563 | EN-GJS-500-7 |
| JIS G5502 | FCD500 |
| UNI 4544 | GS500-7 |
| AS 1831 | 500-7 |
| SAE J434 | D500 |
| SS 14 07 | 0727-02 |
| BS 2789 | 500/7 |
| IS 1865 | SG500/7 |
| UNE 36-118 | FGE50-7 |
| ASTM A536 | 70-50-05 |
| DIN 1693-1 DIN 1693-2 | GGG-50 |
| GB/T 1348 | QT500-7 |
Approximate materials; not guaranteed interchangeable.
Similar Materials
Not Available
Reference Standards
| Standard | Standard Title | Edition | Specification |
|---|---|---|---|
| ISO 1083 | Spheroidal graphite cast irons — Classification | 2018 | ISO1083/JS/500-7 |
Related Casting Products
Physical Properties
| Property | Value | Applicable Conditions |
|---|---|---|
| Density | 7.1 kg/dm³[2] | Room temperature unless otherwise specified |
| Elastic Modulus | 169 GN/m²[2] | Room temperature unless otherwise specified |
| Poisson Ratio | 0.275[2] | Room temperature unless otherwise specified |
| Thermal Conductivity | 35.2 W/(m·K)[2] | Test temperature: 300 °C |
| Specific Heat | 515 J/(kg·K)[2] | Temperature range: 20–500 °C |
| Thermal Expansion | 12.5 µm/(m·K)[2] | Temperature range: 20–400 °C |
| Electrical Resistivity | 0.51 µΩ·m[2] | Room temperature unless otherwise specified |
| Hysteresis Loss | 1345 J/m³[2] | Hysteresis loss at B = 1 T; Room temperature unless otherwise specified |
| Matrix Structure | ferrite-pearlite[1][2] | |
| Maximum Magnetic Permeability | 1596 µH/m[2] | Room temperature unless otherwise specified |
Notes
- [1] Matrix Structure: Typical structure
- [2] Informative values; not mandatory acceptance limits.
Chemical Composition
Not Available
Heat Treatment
ISO 1083–2018
Not Available
Mechanical Properties
Primary Mechanical Properties
ISO 1083 — 2018
| Property | t ≤ 30 mm | 30 < t ≤ 60 mm | 60 < t ≤ 200 mm |
|---|---|---|---|
| Yield Strength (Rp0.2) | ≥ 320 MPa[1][2][3] | ≥ 300 MPa[1][2][3] | ≥ 290 MPa[1][2][3] |
| Tensile Strength | ≥ 500 MPa[1][2][3] | ≥ 450 MPa[1][2][3] | ≥ 420 MPa[1][2][3] |
| Elongation | ≥ 7 %[1][2][3][4][5] | ≥ 7 %[1][2][3][4][5] | ≥ 5 %[1][2][3][4][5] |
Notes
- [1] Separately cast, cast-on or side-by-side cast samples
- [2] Values apply to sand moulds or moulds of comparable thermal behaviour
- [3] alternative processes are subject to amendments agreed in the order.
- [4] Elongation: Elongation values determined from L0 = 5 d
- [5] Elongation: other gauge lengths see 9.1 and Annex B.
ISO 1083 — 2018
Informative
| Property | t ≤ 30 mm | 30 < t ≤ 60 mm | 60 < t ≤ 200 mm |
|---|---|---|---|
| Yield Strength (Rp0.2) | ≥ 300 MPa[1][2][3] | ≥ 280 MPa[1][2][3] | ≥ 260 MPa[1][2][3] |
| Tensile Strength | ≥ 480 MPa[1][2][3] | ≥ 450 MPa[1][2][3] | ≥ 400 MPa[1][2][3] |
| Elongation | ≥ 6 %[1][2][3][4] | ≥ 5 %[1][2][3][4] | ≥ 3 %[1][2][3][4] |
Notes
- [1] test pieces machined from samples cut from castings
- [2] Informative reference value
- [3] not an acceptance requirement
- [4] Elongation: For elongation results, the reference gauge length is L0 = 5 d.
ISO 1083 — 2018
Informative
Notes
- [1] Room temperature unless otherwise specified.
- [2] Informative reference value
- [3] not an acceptance requirement
Additional Mechanical Properties
ISO 1083 — 2018
Other Mechanical Properties
Informative
Notes
- [1] Room temperature unless otherwise specified.
- [2] Informative reference value
- [3] not an acceptance requirement
ISO 1083 — 2018
Fatigue Properties
Informative
| Property | Value |
|---|---|
| Reversed Tension Compression Fatigue Strength | 200 MPa[1][2][3][4][5][6] |
| Reversed Tension Compression Fatigue Ratio | 0.40[1][2][3][4][5][6] |
| Pulsating Tension Fatigue Strength | 280 MPa[1][2][3][4][5][6] |
| Reversed Torsional Fatigue Strength | 180 MPa[1][2][3][4][5][6] |
| Reversed Torsional Fatigue Ratio | 0.36[1][2][3][4][5][6] |
| Rotating Bending Fatigue Strength | 225 MPa[1][2][3][4][5][6] |
| Rotating Bending Fatigue Ratio | 0.45[1][2][3][4][5][6] |
| Notched Rotating Bending Fatigue Strength | 150 MPa[1][2][4][5][6][7] |
| Notched Rotating Bending Fatigue Ratio | 0.30[1][2][4][5][6][7] |
Notes
- [1] specimens diameter <=25 mm from casting
- [2] relevant wall thickness <=30 mm
- [3] Reversed Tension Compression Fatigue Strength; Reversed Tension Compression Fatigue Ratio; Pulsating Tension Fatigue Strength; Reversed Torsional Fatigue Strength; Reversed Torsional Fatigue Ratio; Rotating Bending Fatigue Strength; Rotating Bending Fatigue Ratio: Unnotched specimen
- [4] 10 million cycles and 50% failure probability.
- [5] Informative reference value
- [6] not an acceptance requirement
- [7] Notched Rotating Bending Fatigue Strength; Notched Rotating Bending Fatigue Ratio: Notched specimen with stress concentration factor Kt ≤ 3
Welding Conditions
Not Available
Applications
Ductile iron ISO1083/JS/500-7 belongs to the spheroidal graphite iron casting family. Foundry applications for spheroidal graphite iron include gears, support brackets, wheel hubs and casings for industrial pumps. Manufacturers supply such castings for agricultural equipment, vehicle assemblies and flow-control machinery.
Need ISO1083/JS/500-7 Castings?
Contact us for casting and machining inquiries.
Email Us for a QuoteLast Updated: November 16, 2026