ISO1083/JS/600-3 Ductile Cast Iron Casting Material
Ductile Cast Iron
Introduction
ISO1083/JS/600-3 is an ISO 1083 grade of spheroidal graphite cast iron. The standard reports pearlite-ferrite as a typical matrix. Typical family castings include bearing housings and pump components.
| Field | Value |
|---|---|
| Designation | ISO1083/JS/600-3 |
| Material Type | Cast Iron |
| Sub Type | Ductile Cast Iron |
| Product Form | casting |
Manufacturing Process
Sand Casting
Shell Molding Casting
Lost Foam Casting
Equivalent Materials
| Standard | Material Grade |
|---|---|
| UNI 4544 | GS600-2 |
| NS11 301 | SJK-600 |
| BS 2789 | 600/7 |
| IS 1865 | SG600/3 |
| EN 1563 | EN-GJS-600-3 |
| NF A32-201 | FGS600-2 |
| AS 1831 | 600-3 |
| NBN 830-02 | FNG60-2 |
| JIS G5502 | FCD600 |
| UNE 36-118 | FGE60-2 |
| SS 14 07 | 0732-03 |
| DIN 1693-1 DIN 1693-2 | GGG-60 |
| GB/T 1348 | QT600-3 |
Approximate materials; not guaranteed interchangeable.
Similar Materials
Not Available
Reference Standards
| Standard | Standard Title | Edition | Specification |
|---|---|---|---|
| ISO 1083 | Spheroidal graphite cast irons — Classification | 2018 | ISO1083/JS/600-3 |
Related Casting Products
Physical Properties
| Property | Value | Applicable Conditions |
|---|---|---|
| Density | 7.2 kg/dm³[2] | Room temperature unless otherwise specified |
| Elastic Modulus | 174 GN/m²[2] | Room temperature unless otherwise specified |
| Poisson Ratio | 0.275[2] | Room temperature unless otherwise specified |
| Thermal Conductivity | 32.5 W/(m·K)[2] | Test temperature: 300 °C |
| Specific Heat | 515 J/(kg·K)[2] | Temperature range: 20–500 °C |
| Thermal Expansion | 12.5 µm/(m·K)[2] | Temperature range: 20–400 °C |
| Electrical Resistivity | 0.53 µΩ·m[2] | Room temperature unless otherwise specified |
| Hysteresis Loss | 2248 J/m³[2] | Hysteresis loss at B = 1 T; Room temperature unless otherwise specified |
| Matrix Structure | pearlite-ferrite[1][2] | |
| Maximum Magnetic Permeability | 866 µH/m[2] | Room temperature unless otherwise specified |
Notes
- [1] Matrix Structure: Typical structure
- [2] Informative values; not mandatory acceptance limits.
Chemical Composition
Not Available
Heat Treatment
ISO 1083–2018
Not Available
Mechanical Properties
Primary Mechanical Properties
ISO 1083 — 2018
| Property | t ≤ 30 mm | 30 < t ≤ 60 mm | 60 < t ≤ 200 mm |
|---|---|---|---|
| Yield Strength (Rp0.2) | ≥ 370 MPa[1][2][3] | ≥ 360 MPa[1][2][3] | ≥ 340 MPa[1][2][3] |
| Tensile Strength | ≥ 600 MPa[1][2][3] | ≥ 600 MPa[1][2][3] | ≥ 550 MPa[1][2][3] |
| Elongation | ≥ 3 %[1][2][3][4][5] | ≥ 2 %[1][2][3][4][5] | ≥ 1 %[1][2][3][4][5] |
Notes
- [1] Separately cast, cast-on or side-by-side cast samples
- [2] Values apply to sand moulds or moulds of comparable thermal behaviour
- [3] alternative processes are subject to amendments agreed in the order.
- [4] Elongation: Elongation values determined from L0 = 5 d
- [5] Elongation: other gauge lengths see 9.1 and Annex B.
ISO 1083 — 2018
Informative
| Property | t ≤ 30 mm | 30 < t ≤ 60 mm | 60 < t ≤ 200 mm |
|---|---|---|---|
| Yield Strength (Rp0.2) | ≥ 360 MPa[1][2][3] | ≥ 340 MPa[1][2][3] | ≥ 320 MPa[1][2][3] |
| Tensile Strength | ≥ 580 MPa[1][2][3] | ≥ 550 MPa[1][2][3] | ≥ 500 MPa[1][2][3] |
| Elongation | ≥ 3 %[1][2][3][4] | ≥ 2 %[1][2][3][4] | ≥ 1 %[1][2][3][4] |
Notes
- [1] test pieces machined from samples cut from castings
- [2] Informative reference value
- [3] not an acceptance requirement
- [4] Elongation: For elongation results, the reference gauge length is L0 = 5 d.
ISO 1083 — 2018
Informative
Notes
- [1] Room temperature unless otherwise specified.
- [2] Informative reference value
- [3] not an acceptance requirement
Additional Mechanical Properties
ISO 1083 — 2018
Other Mechanical Properties
Informative
Notes
- [1] Room temperature unless otherwise specified.
- [2] Informative reference value
- [3] not an acceptance requirement
ISO 1083 — 2018
Fatigue Properties
Informative
| Property | Value |
|---|---|
| Reversed Tension Compression Fatigue Strength | 228 MPa[1][2][3][4][5][6] |
| Reversed Tension Compression Fatigue Ratio | 0.38[1][2][3][4][5][6] |
| Pulsating Tension Fatigue Strength | 319 MPa[1][2][3][4][5][6] |
| Reversed Torsional Fatigue Strength | 204 MPa[1][2][3][4][5][6] |
| Reversed Torsional Fatigue Ratio | 0.34[1][2][3][4][5][6] |
| Rotating Bending Fatigue Strength | 258 MPa[1][2][3][4][5][6] |
| Rotating Bending Fatigue Ratio | 0.43[1][2][3][4][5][6] |
| Notched Rotating Bending Fatigue Strength | 168 MPa[1][2][4][5][6][7] |
| Notched Rotating Bending Fatigue Ratio | 0.28[1][2][4][5][6][7] |
Notes
- [1] specimens diameter <=25 mm from casting
- [2] relevant wall thickness <=30 mm
- [3] Reversed Tension Compression Fatigue Strength; Reversed Tension Compression Fatigue Ratio; Pulsating Tension Fatigue Strength; Reversed Torsional Fatigue Strength; Reversed Torsional Fatigue Ratio; Rotating Bending Fatigue Strength; Rotating Bending Fatigue Ratio: Unnotched specimen
- [4] 10 million cycles and 50% failure probability.
- [5] Informative reference value
- [6] not an acceptance requirement
- [7] Notched Rotating Bending Fatigue Strength; Notched Rotating Bending Fatigue Ratio: Notched specimen with stress concentration factor Kt ≤ 3
Welding Conditions
Not Available
Applications
Ductile iron ISO1083/JS/600-3 belongs to the spheroidal graphite iron casting family. Ductile-iron foundries make gears, hubs and brackets alongside pump casings and bearing housings for engineering equipment. Examples of end-use sectors include general industrial machinery, agriculture, construction and pump equipment.