Introduction
GB/T 1348 Grade QT700-2 is a spheroidal graphite iron casting grade. Process options include sand casting, shell molding and lost-foam casting. Typical uses include gear blanks, transmission components, crankshafts and machinery parts.
| Field | Value |
|---|---|
| Designation | QT700-2 |
| Material Type | Cast Iron |
| Sub Type | Ductile Cast Iron |
| Product Form | casting |
Manufacturing Process
Sand Casting
Shell Molding Casting
Lost Foam Casting
Equivalent Materials
| Standard | Material Grade |
|---|---|
| EN 1563 | EN-GJS-700-2 |
| AS 1831 | 700-2 |
| UNE 36-118 | FGE70-2 |
| NS11 301 | SJK-700 |
| JIS G5502 | FCD700 |
| UNI 4544 | GS700-2 |
| SS 14 07 | 0737-01 |
| SAE J434 | D700 |
| NF A32-201 | FGS700-2 |
| BS 2789 | 700/2 |
| NBN 830-02 | FNG70-2 |
| IS 1865 | SG700/2 |
| ASTM A536 | 100-70-03 |
| DIN 1693-1 DIN 1693-2 | GGG-70 |
| ISO 1083 | ISO1083/JS/700-2 |
Approximate materials; not guaranteed interchangeable.
Similar Materials
Not Available
Reference Standards
| Standard | Standard Title | Edition | Specification |
|---|---|---|---|
| GB/T 1348 | Spheroidal graphite iron castings | 2019 | QT700-2 |
Related Casting Products
Physical Properties
| Property | Value | Applicable Conditions |
|---|---|---|
| Density | 7.2 kg/dm³[1] | Room temperature unless otherwise stated |
| Elastic Modulus | 176 GPa[1] | Room temperature unless otherwise stated |
| Poisson Ratio | 0.275[1] | Room temperature unless otherwise stated |
| Thermal Conductivity | 31.1 W/(m·K)[1] | Test temperature: 300 °C |
| Specific Heat | 515 J/(kg·K)[1] | Temperature range: 20–500 °C |
| Thermal Expansion | 12.5 ×10⁻⁶/K[1] | Temperature range: 20–400 °C |
| Electrical Resistivity | 0.54 µΩ·m[1] | Room temperature unless otherwise stated |
| Hysteresis Loss | 2700 J/m³[1] | Room temperature unless otherwise stated; B = 1 T |
| Matrix Structure | Pearlitic; for large castings see original footnote a for other listed matrix structures; informative Table G.1 matrix description, not a prescribed heat-treatment schedule.[1] | |
| Maximum Magnetic Permeability | 501 µH/m[1] | Room temperature unless otherwise stated |
Notes
- [1] Informative values; not mandatory acceptance limits.
Chemical Composition
No specified chemical composition limits in GB/T 1348
Heat Treatment
General casting and chemical requirements — No grade-specific heat-treatment temperature or holding schedule is prescribed. Alloy adjustment or heat treatment may control the ferrite/pearlite ratio (6.2). When heat treatment is required, test blocks receive the same treatment as the represented castings; cast-on blocks remain attached until after heat treatment unless agreed otherwise (8.1.6; 8.2.3.5; 8.2.5.5). Repeated heat treatments for retesting shall not exceed two (10.5.3).
Mechanical Properties
Primary Mechanical Properties
GB/T 1348 — 2019
Condition: Table 1; Separately cast, cast-on or side-by-side cast sample; 30 < t ≤ 60 mm; normative; 30 < t ≤ 60 mm
| Property | Requirement |
|---|---|
| Yield Strength (Rp0.2) | ≥ 400 MPa[1][2][3][4] |
| Tensile Strength | ≥ 700 MPa[1][2][3][4] |
| Elongation | ≥ 2 %[1][2][3][4] |
Notes
- [1] Table 1: results from cast samples do not directly represent casting-body properties. Separately cast, cast-on and side-by-side cast samples are covered. L denotes low temperature and R room temperature. Elongation is measured at original gauge length L0=5d; alternate gauge lengths require the provisions of 9.1 and normative Annex D.
- [2] Gauge Length: L0 = 5d
- [3] GB/T 228.1
- [4] Minimum prescribed value
GB/T 1348 — 2019
Condition: Table 1; Separately cast, cast-on or side-by-side cast sample; 60 < t ≤ 200 mm; normative; 60 < t ≤ 200 mm
| Property | Requirement |
|---|---|
| Yield Strength (Rp0.2) | ≥ 380 MPa[1][2][3][4] |
| Tensile Strength | ≥ 650 MPa[1][2][3][4] |
| Elongation | ≥ 1 %[1][2][3][4] |
Notes
- [1] Table 1: results from cast samples do not directly represent casting-body properties. Separately cast, cast-on and side-by-side cast samples are covered. L denotes low temperature and R room temperature. Elongation is measured at original gauge length L0=5d; alternate gauge lengths require the provisions of 9.1 and normative Annex D.
- [2] Gauge Length: L0 = 5d
- [3] GB/T 228.1
- [4] Minimum prescribed value
GB/T 1348 — 2019
Condition: Table 1; Separately cast, cast-on or side-by-side cast sample; t ≤ 30 mm; normative; t ≤ 30 mm
| Property | Requirement |
|---|---|
| Yield Strength (Rp0.2) | ≥ 420 MPa[1][2][3][4] |
| Tensile Strength | ≥ 700 MPa[1][2][3][4] |
| Elongation | ≥ 2 %[1][2][3][4] |
Notes
- [1] Table 1: results from cast samples do not directly represent casting-body properties. Separately cast, cast-on and side-by-side cast samples are covered. L denotes low temperature and R room temperature. Elongation is measured at original gauge length L0=5d; alternate gauge lengths require the provisions of 9.1 and normative Annex D.
- [2] Gauge Length: L0 = 5d
- [3] GB/T 228.1
- [4] Minimum prescribed value
GB/T 1348 — 2019
Condition: Table C.1; Specimen cut from the casting; source designation QT700-2/C; sampling position and acceptance properties subject to agreement; 30 < t ≤ 60 mm; informative; 30 < t ≤ 60 mm
Informative
| Property | Value |
|---|---|
| Yield Strength (Rp0.2) | ≥ 390 MPa[1][2][3][4][5][6] |
| Tensile Strength | ≥ 650 MPa[1][2][3][4][5][6] |
| Elongation | ≥ 1 %[1][2][3][4][5][6] |
Notes
- [1] informative 30 < wall thickness ≤ 60 mm
- [2] Gauge Length: L0 = 5d
- [3] GB/T 228.1
- [4] Informative minimum guideline, not an unconditional acceptance requirement
- [5] Informative reference value
- [6] not an acceptance requirement
GB/T 1348 — 2019
Condition: Table C.1; Specimen cut from the casting; source designation QT700-2/C; sampling position and acceptance properties subject to agreement; 60 < t ≤ 200 mm; informative; 60 < t ≤ 200 mm
Informative
| Property | Value |
|---|---|
| Yield Strength (Rp0.2) | ≥ 370 MPa[1][2][3][4][5][6] |
| Tensile Strength | ≥ 600 MPa[1][2][3][4][5][6] |
| Elongation | ≥ 1 %[1][2][3][4][5][6] |
Notes
- [1] informative 60 < wall thickness ≤ 200 mm
- [2] Gauge Length: L0 = 5d
- [3] GB/T 228.1
- [4] Informative minimum guideline, not an unconditional acceptance requirement
- [5] Informative reference value
- [6] not an acceptance requirement
GB/T 1348 — 2019
Condition: Table C.1; Specimen cut from the casting; source designation QT700-2/C; sampling position and acceptance properties subject to agreement; t ≤ 30 mm; informative; t ≤ 30 mm
Informative
| Property | Value |
|---|---|
| Yield Strength (Rp0.2) | ≥ 410 MPa[1][2][3][4][5][6] |
| Tensile Strength | ≥ 680 MPa[1][2][3][4][5][6] |
| Elongation | ≥ 2 %[1][2][3][4][5][6] |
Notes
- [1] informative wall thickness ≤ 30 mm
- [2] Gauge Length: L0 = 5d
- [3] GB/T 228.1
- [4] Informative minimum guideline, not an unconditional acceptance requirement
- [5] Informative reference value
- [6] not an acceptance requirement
GB/T 1348 — 2019
Condition: Table G.1; informative
Informative
Notes
- [1] Annex G informative reference data
- [2] measured at room temperature unless otherwise stated, not an acceptance limit
- [3] Informative reference value
- [4] not an acceptance requirement
GB/T 1348 — 2019
Condition: t ≤ 30 mm; Table G.2; Specimen cut from casting; diameter ≤25 mm; t ≤ 30 mm; informative
Informative
Notes
- [1] Informative guideline
- [2] stress-controlled fatigue
- [3] N = 10^7 cycles, failure probability P = 50% for fatigue data
- [4] not an acceptance requirement
- [5] Informative reference value
Additional Mechanical Properties
GB/T 1348 — 2019
Other Mechanical Properties
Condition: Table G.1; informative
Informative
Notes
- [1] Annex G informative reference data
- [2] measured at room temperature unless otherwise stated, not an acceptance limit
- [3] Informative reference value
- [4] not an acceptance requirement
GB/T 1348 — 2019
Fracture Toughness
Condition: Table G.1; informative
Informative
Notes
- [1] Annex G informative reference data
- [2] measured at room temperature unless otherwise stated, not an acceptance limit
- [3] Informative reference value
- [4] not an acceptance requirement
GB/T 1348 — 2019
Fatigue Properties
Condition: t ≤ 30 mm
Informative
| Property | Value |
|---|---|
| Notched Rotating Bending Fatigue Strength | 182 MPa[1][2][3][4][5][6][7][8][9][10][11][12][13][14][15][16] |
| Notched Rotating Bending Fatigue Ratio | 0.26[1][2][3][4][5][6][7][8][9][10][11][17] |
| Reversed Tension Compression Fatigue Strength | 252 MPa[1][3][4][5][6][7][8][9][10][11][12][16][18][19][20] |
| Reversed Tension Compression Fatigue Ratio | 0.36[1][3][4][5][6][7][8][9][10][11][17][18] |
| Pulsating Tension Fatigue Strength | 353 MPa[1][3][4][5][6][7][8][9][10][11][16][18][21][22][23][24] |
| Reversed Torsional Fatigue Strength | 224 MPa[1][3][4][5][6][7][8][9][10][11][12][16][18][25][26] |
| Reversed Torsional Fatigue Ratio | 0.32[1][3][4][5][6][7][8][9][10][11][17][18] |
| Rotating Bending Fatigue Strength | 287 MPa[1][3][4][5][6][7][8][9][10][11][12][16][18][27][28] |
| Rotating Bending Fatigue Ratio | 0.41[1][3][4][5][6][7][8][9][10][11][17][18] |
Notes
- [1] GB/T 1348:2019 G.2 prints contradictory cycle wording. With owner authorization, adopt 10 million cycles (N=10^7), P=50% from verified ISO 1083:2018 G.2 footnotes b/c. This is separately sourced supporting clarification, not an official amendment or mandatory acceptance value.
- [2] Notched Rotating Bending Fatigue Strength; Notched Rotating Bending Fatigue Ratio: Notched specimen, Kt ≤3 machined from a sample cut from casting
- [3] diameter ≤25 mm
- [4] relevant wall thickness t ≤30 mm
- [5] informative wall thickness ≤ 30 mm
- [6] Informative guidance, not an acceptance requirement
- [7] GB cycle wording retained as inconsistent
- [8] N = 10^7 cycles (10 million), P = 50% adopted from ISO 1083:2018 G.2 footnotes b/c under owner authorization
- [9] Stress-controlled fatigue according to Wöhler
- [10] Informative reference value
- [11] not an acceptance requirement
- [12] Notched Rotating Bending Fatigue Strength; Reversed Tension Compression Fatigue Strength; Reversed Torsional Fatigue Strength; Rotating Bending Fatigue Strength: R = -1
- [13] Notched Rotating Bending Fatigue Strength: approximately 21.8%
- [14] Notched Rotating Bending Fatigue Strength: Kt ≤ 3
- [15] Notched Rotating Bending Fatigue Strength: σbwk(R=-1)/Rm ≈ 0.40 - 0.0002 × Rm
- [16] Notched Rotating Bending Fatigue Strength; Reversed Tension Compression Fatigue Strength; Pulsating Tension Fatigue Strength; Reversed Torsional Fatigue Strength; Rotating Bending Fatigue Strength: Mean source-table reference strength, not a guaranteed limit
- [17] Notched Rotating Bending Fatigue Ratio; Reversed Tension Compression Fatigue Ratio; Reversed Torsional Fatigue Ratio; Rotating Bending Fatigue Ratio: Source-table ratio, not a calculated value
- [18] Reversed Tension Compression Fatigue Strength; Reversed Tension Compression Fatigue Ratio; Pulsating Tension Fatigue Strength; Reversed Torsional Fatigue Strength; Reversed Torsional Fatigue Ratio; Rotating Bending Fatigue Strength; Rotating Bending Fatigue Ratio: Unnotched specimen machined from a sample cut from casting
- [19] Reversed Tension Compression Fatigue Strength: approximately 22.3%
- [20] Reversed Tension Compression Fatigue Strength: σw/Rm ≈ 0.50 - 0.0002 × Rm
- [21] Pulsating Tension Fatigue Strength: R = 0
- [22] Pulsating Tension Fatigue Strength: σmax = 2σ
- [23] Pulsating Tension Fatigue Strength: approximately 9%
- [24] Pulsating Tension Fatigue Strength: σ(R=0)/σ(R=-1) ≈ 0.7
- [25] Reversed Torsional Fatigue Strength: approximately 14%
- [26] Reversed Torsional Fatigue Strength: τw/Rm ≈ 0.46 - 0.0002 × Rm
- [27] Rotating Bending Fatigue Strength: approximately 14.2%
- [28] Rotating Bending Fatigue Strength: σw/Rm ≈ 0.55 - 0.0002 × Rm
Welding Conditions
Not Available
Applications
Ductile iron GB/T 1348 Grade QT700-2 is used for gear blanks, transmission components, crankshafts and machinery parts. Such castings are used in industrial drives, agricultural machinery, engines and off-highway equipment. Component selection depends on section size, loading and the required finished surface. Wear performance or fatigue life cannot be inferred from the grade name alone; any surface treatment and associated acceptance requirements must be specified for the actual part.
Need QT700-2 Castings?