ISO1083/JS/350-22 Ductile Cast Iron Casting Material

Ductile Cast Iron

Download MDS PDF · Request a Quote

Introduction

ISO1083/JS/350-22 is a spheroidal graphite cast iron specified in ISO 1083. The standard reports ferrite as a typical matrix. The wider ductile-iron family is used for pump casings and machinery housings.

FieldValue
DesignationISO1083/JS/350-22
Material TypeCast Iron
Sub TypeDuctile Cast Iron
Product Formcasting

Manufacturing Process

Sand Casting
Shell Molding Casting
Lost Foam Casting

Equivalent Materials

StandardMaterial Grade
EN 1563EN-GJS-350-22
GB/T 1348QT350-22

Approximate materials; not guaranteed interchangeable.

Similar Materials

Not Available

Reference Standards

StandardStandard TitleEditionSpecification
ISO 1083Spheroidal graphite cast irons — Classification2018ISO1083/JS/350-22

Physical Properties

PropertyValueApplicable Conditions
Density7.1 kg/dm³[2]Room temperature unless otherwise specified
Elastic Modulus169 GN/m²[2]Room temperature unless otherwise specified
Poisson Ratio0.275[2]Room temperature unless otherwise specified
Thermal Conductivity36.2 W/(m·K)[2]Test temperature: 300 °C
Specific Heat515 J/(kg·K)[2]Temperature range: 20–500 °C
Thermal Expansion12.5 µm/(m·K)[2]Temperature range: 20–400 °C
Electrical Resistivity0.50 µΩ·m[2]Room temperature unless otherwise specified
Hysteresis Loss600 J/m³[2]Hysteresis loss at B = 1 T; Room temperature unless otherwise specified
Matrix Structureferrite[1][2]
Maximum Magnetic Permeability2136 µH/m[2]Room temperature unless otherwise specified

Notes

  • [1] Matrix Structure: Typical structure
  • [2] Informative values; not mandatory acceptance limits.

Chemical Composition

Not Available

Heat Treatment

ISO 1083–2018

Not Available

Mechanical Properties

Primary Mechanical Properties

ISO 1083 — 2018

Propertyt ≤ 30 mm30 < t ≤ 60 mm60 < t ≤ 200 mm
Yield Strength (Rp0.2)≥ 220 MPa[1][2][3]≥ 220 MPa[1][2][3]≥ 210 MPa[1][2][3]
Tensile Strength≥ 350 MPa[1][2][3]≥ 330 MPa[1][2][3]≥ 320 MPa[1][2][3]
Elongation≥ 22 %[1][2][3][4][5]≥ 18 %[1][2][3][4][5]≥ 15 %[1][2][3][4][5]

Notes

  • [1] Separately cast, cast-on or side-by-side cast samples
  • [2] Values apply to sand moulds or moulds of comparable thermal behaviour
  • [3] alternative processes are subject to amendments agreed in the order.
  • [4] Elongation: Elongation values determined from L0 = 5 d
  • [5] Elongation: other gauge lengths see 9.1 and Annex B.

ISO 1083 — 2018

Informative

Propertyt ≤ 30 mm30 < t ≤ 60 mm60 < t ≤ 200 mm
Yield Strength (Rp0.2)≥ 220 MPa[1][2][3]≥ 210 MPa[1][2][3]≥ 200 MPa[1][2][3]
Tensile Strength≥ 340 MPa[1][2][3]≥ 320 MPa[1][2][3]≥ 310 MPa[1][2][3]
Elongation≥ 20 %[1][2][3][4]≥ 15 %[1][2][3][4]≥ 12 %[1][2][3][4]

Notes

  • [1] test pieces machined from samples cut from castings
  • [2] Informative reference value
  • [3] not an acceptance requirement
  • [4] Elongation: For elongation results, the reference gauge length is L0 = 5 d.

ISO 1083 — 2018

Informative

PropertyValue
Shear Strength315 MPa[1][2][3]

Notes

  • [1] Room temperature unless otherwise specified.
  • [2] Informative reference value
  • [3] not an acceptance requirement

ISO 1083 — 2018

Informative

PropertyValue
Tensile Strength350 MPa[1][2][3][4]

Notes

  • [1] specimens diameter <=25 mm from casting
  • [2] relevant wall thickness <=30 mm
  • [3] Informative reference value
  • [4] not an acceptance requirement

Additional Mechanical Properties

ISO 1083 — 2018

Other Mechanical Properties

Informative

PropertyValue
Torsional Strength315 MPa[1][2][3]

Notes

  • [1] Room temperature unless otherwise specified.
  • [2] Informative reference value
  • [3] not an acceptance requirement

ISO 1083 — 2018

Fatigue Properties

Informative

PropertyValue
Reversed Tension Compression Fatigue Strength150 MPa[1][2][3][4][5][6]
Reversed Tension Compression Fatigue Ratio0.43[1][2][3][4][5][6]
Pulsating Tension Fatigue Strength210 MPa[1][2][3][4][5][6]
Reversed Torsional Fatigue Strength138 MPa[1][2][3][4][5][6]
Reversed Torsional Fatigue Ratio0.39[1][2][3][4][5][6]
Rotating Bending Fatigue Strength168 MPa[1][2][3][4][5][6]
Rotating Bending Fatigue Ratio0.48[1][2][3][4][5][6]
Notched Rotating Bending Fatigue Strength115 MPa[1][2][4][5][6][7]
Notched Rotating Bending Fatigue Ratio0.33[1][2][4][5][6][7]

Notes

  • [1] specimens diameter <=25 mm from casting
  • [2] relevant wall thickness <=30 mm
  • [3] Reversed Tension Compression Fatigue Strength; Reversed Tension Compression Fatigue Ratio; Pulsating Tension Fatigue Strength; Reversed Torsional Fatigue Strength; Reversed Torsional Fatigue Ratio; Rotating Bending Fatigue Strength; Rotating Bending Fatigue Ratio: Unnotched specimen
  • [4] 10 million cycles and 50% failure probability.
  • [5] Informative reference value
  • [6] not an acceptance requirement
  • [7] Notched Rotating Bending Fatigue Strength; Notched Rotating Bending Fatigue Ratio: Notched specimen with stress concentration factor Kt ≤ 3

Welding Conditions

Not Available

Applications

Ductile iron ISO1083/JS/350-22 belongs to the spheroidal graphite iron casting family. Within this material family, foundries produce pump casings, bearing housings, valve bodies and cover plates for machinery. These types of components occur in agricultural machinery, construction equipment and industrial fluid-handling systems.

Need ISO1083/JS/350-22 Castings?

Contact us for casting and machining inquiries.

Last Updated: November 16, 2026