GX40NiCrSiNb35-26 (EN 1.4852) Austenitic Stainless Steel Casting Material
Austenitic Stainless Steel
Introduction
EN 10295 Grade GX40NiCrSiNb35-26 is a heat-resistant austenitic stainless steel casting grade. Process options include investment casting, shell molding and sand casting. Typical uses include oil and gas plant cast components.
| Field | Value |
|---|---|
| Designation | GX40NiCrSiNb35-26 (EN 1.4852) |
| Material Type | Stainless Steel |
| Sub Type | Austenitic Stainless Steel |
| Product Form | casting |
Manufacturing Process
Investment Casting
Shell Molding Casting
Sand Casting
Equivalent Materials
Not Available
Similar Materials
Not Available
Reference Standards
| Standard | Standard Title | Edition | Specification | Identifier |
|---|---|---|---|---|
| EN 10295 | Heat resistant steel castings | 2002 | GX40NiCrSiNb35-26 | EN 1.4852 |
Related Casting Products
Physical Properties
| Property | Value | Applicable Conditions |
|---|---|---|
| Density | 8.0 kg/dm³[1] | |
| Thermal Conductivity | 12.8 W/(m·K)[1] | Test temperature: 20 °C |
| Thermal Conductivity | 13 W/(m·K)[1] | Test temperature: 100 °C |
| Thermal Conductivity | 23.5 W/(m·K)[1] | Test temperature: 800 °C |
| Thermal Conductivity | 27.7 W/(m·K)[1] | Test temperature: 1000 °C |
| Specific Heat | 500 J/(kg·K)[1] | Test temperature: 20 °C |
| Thermal Expansion | 16 ×10⁻⁶/K[1] | Temperature range: 20–400 °C |
| Thermal Expansion | 17.8 ×10⁻⁶/K[1] | Temperature range: 20–800 °C |
| Thermal Expansion | 18.6 ×10⁻⁶/K[1] | Temperature range: 20–1000 °C |
Notes
- [1] Informative values; not mandatory acceptance limits.
Chemical Composition
| Element | Requirement |
|---|---|
| C | 0.30–0.50 %[1] |
| Si | 1.00–2.50 %[1] |
| Mn | ≤ 2.00 %[1] |
| P | ≤ 0.040 %[1] |
| S | ≤ 0.030 %[1] |
| Cr | 24.00–27.00 %[1] |
| Ni | 33.00–36.00 %[1] |
| Mo | ≤ 0.50 %[1] |
| Cu | ≤ 0.25 %[2] |
| V | ≤ 0.12 %[2] |
| Nb | 0.80–1.80 %[1] |
| W | ≤ 0.60 %[2] |
| Co | ≤ 1.00 %[2] |
Notes
- [1] C; Si; Mn; P; S; Cr; Mo; Ni; Nb: cast analysis
- [2] W; V; Cu; Co: Unless otherwise agreed: limit for element unspecified in Table 1; no intentional addition except for finishing the heat.; cast analysis
Heat Treatment
EN 10295–2002
Not Available
Mechanical Properties
Primary Mechanical Properties
EN 10295 — 2002
Condition: Room temperature; As cast / no heat treatment
| Property | Requirement |
|---|---|
| Yield Strength | ≥ 220 MPa[1] |
| Tensile Strength | ≥ 440 MPa |
| Elongation | ≥ 4 % |
Notes
- [1] Yield Strength: Yield strength is 0.2% proof strength.
Additional Mechanical Properties
EN 10295 — 2002
Creep & Stress-Rupture Properties
Condition: 100 h
Informative
| Property | 700 °C | 800 °C | 900 °C | 1000 °C |
|---|---|---|---|---|
| σr — mean rupture stress | 155 MPa[1][2][3][4] | 90 MPa[1][2][3][4] | 49 MPa[1][2][3][4] | 30 MPa[1][2][3][4] |
Notes
- [1] Mean creep values from a scatter band of ±20%; information only.
- [2] Mean values
- [3] ±20% scatter band
- [4] information only, not acceptance requirements
EN 10295 — 2002
Creep & Stress-Rupture Properties
Condition: 100 h; 1100 °C
Informative
Notes
- [1] Mean creep values from a scatter band of ±20%; information only.
- [2] Mean values
- [3] ±20% scatter band
- [4] information only, not acceptance requirements
EN 10295 — 2002
Creep & Stress-Rupture Properties
Condition: 1000 h
Informative
| Property | 700 °C | 800 °C | 900 °C | 1000 °C |
|---|---|---|---|---|
| σr — mean rupture stress | 120 MPa[1][2][3][4] | 70 MPa[1][2][3][4] | 38 MPa[1][2][3][4] | 20 MPa[1][2][3][4] |
Notes
- [1] Mean creep values from a scatter band of ±20%; information only.
- [2] Mean values
- [3] ±20% scatter band
- [4] information only, not acceptance requirements
EN 10295 — 2002
Creep & Stress-Rupture Properties
Condition: 1000 h; 1100 °C
Informative
Notes
- [1] Mean creep values from a scatter band of ±20%; information only.
- [2] Mean values
- [3] ±20% scatter band
- [4] information only, not acceptance requirements
EN 10295 — 2002
Creep & Stress-Rupture Properties
Condition: 10000 h
Informative
| Property | 700 °C | 800 °C | 900 °C | 1000 °C |
|---|---|---|---|---|
| σ1% — mean stress for 1% elongation | 72 MPa[1][2][3][4] | 41 MPa[1][2][3][4] | 22 MPa[1][2][3][4] | 9 MPa[1][2][3][4] |
Notes
- [1] Mean creep values from a scatter band of ±20%; information only.
- [2] Mean values
- [3] ±20% scatter band
- [4] information only, not acceptance requirements
EN 10295 — 2002
Creep & Stress-Rupture Properties
Condition: 10000 h; 1100 °C
Informative
Notes
- [1] Mean creep values from a scatter band of ±20%; information only.
- [2] Mean values
- [3] ±20% scatter band
- [4] information only, not acceptance requirements
Welding Conditions
Not Available
Applications
Austenitic stainless steel EN 10295 GX40NiCrSiNb35-26 is typically used for oil and gas plant cast components. EN 10295:2002 gives an informative maximum use temperature in air of 1100 °C, based on oxidation resistance in clean natural air. These figures are not guaranteed continuous or intermittent service temperatures, or allowable temperatures under load; other atmospheres require separate assessment.
Other cast components used in this material family include furnace fixtures, support elements and burner-assembly components. These applications include industrial heating and heat-treatment equipment. Atmosphere, loading, direct flame exposure, cyclic operation and process deposits must be considered separately from an in-air reference temperature.
Need GX40NiCrSiNb35-26 Castings?
Contact us for casting and machining inquiries.