ISO3755, 230-450 230-450W Carbon Steel
Casting grades: 230-450 230-450W
Metal Type: Carbon Steels
Casting Process: Sand Casting or Lost Wax Precision Investment Casting
Standard: ISO 3755
Similar Grade: GBT11352 ZG230-450; ASTM A27 450-240; BS3100 AM2; DIN1681 GS45 JIS5101 SC450; ГОСТ 977 25Л
Heat treatment: Annealing, Quenching and Tempering
Steel Grade | C % | Mn % | Si % | P % | S % | Ni % | Cr % | Cu % | Mo % | V % |
230-450 | – | – | – | 0.035 | 0.035 | – | – | – | – | |
230-450W | 0.25 | 1.20 | 0.60 | 0.035 | 0.035 | 0.40 | 0.35 | 0.40 | 0.15 | 0.05 |
Steel Grade | Tensile Strength Rm Mpa | Upper Yield Re, Mpa | Elongation % | Reduction of area Z % | Impact Strength KV J |
230-450 | 450-600 | 230 | 22 | 31 | 25 |
230-450W | 450-600 | 230 | 22 | 31 | 45 |
1. Mechanical properties are obtained from 28mm thick standard test blocks.
2. The testing ambient temperature was take as 23 ±- 5°C degree
What’s the means “W” in ISO3755?
“W” means WELDABLE GRADE. For example, 230-450 is non-weldable grade casting materiel, it’s choice of chemical composition shall be left to the discretion of the manufacturer. But 230-450W is weldable grade, ISO 3755 standard indicate the detailed chemistry for welding purpose.